PMMA V045-100 法國阿托菲納公司 物性數據 |
規格級別: | 耐熱級 | 外觀顏色: | --- |
用途概述: | --- | ||
備注說明: | --- |
性能項目 | 試驗條件[狀態] | 測試方法 | 測試數據 | 數據單位 | |
基本性能 | 熔體流動速率 | --- | ASTM D-1238 | 2.3 | g/10min |
吸水率 | 浸水24hrs后增重 | ASTM D-570 | 0.3 | % | |
物理性能 | 成形收縮率 | (冷模/冷件),48hrs | ASTM D-935 | 0.2-0.6 | % |
透光率 | --- | ASTM D-1003 | 92 | % | |
折射率ND | --- | ASTM D-542 | 1.49 | --- | |
比重 | --- | ASTM D-792 | 1.19 | --- | |
霧度 | --- | --- | <2 | % | |
機械性能 | 洛氏硬度 | --- | ASTM D-758 | 96 | M scale |
拉伸強度 | 初級應變速率0.1cm/cm/min | ASTM D-638 | 720(70) | kgf/cm2 | |
彎曲強度 | 橫跨比=16 | ASTM D-790 | 1050(103) | kgf/cm2(MPa) | |
彎曲模數 | --- | ASTM D-790 | 32000 | kgf/cm2 | |
沖擊強度 | Izod研磨缺口 | ASTM D-256 | 1.2(12.3) | kgf.cm/cm(J/m) | |
沖擊強度 | 落錘(15.2×15.2×0.3cm重1.4kg半徑0.64cm) | ASTM D-256 | 14(1.4) | kg.cm(J) | |
熱 性 能 | 熱變形溫度負荷,退火 | 2℃/min,18.6kgf/cm2 | ASTM D-648 | 93 | ℃ |
維卡軟化點 | 未退火,50℃/hr,1kg | ASTM D-1525 | 103 | ℃ | |
維卡軟化點 | 未退火,50℃/hr,5kg | ASTM D-1525 | 97 | ℃ | |
玻璃化轉變溫度Tg | --- | --- | 104 | ℃ | |
使用溫度范圍 | 與殘余應力大小有關 | --- | 74-88 | ℃ |